Microstructure and Properties of CBN Abrasive Blocks with Cu-Sn-Ti Binder Modified by Ceramic Glass Powder.
Huiju Zhang, Duanzhi Duan, Congcong Cao, Chunhui Li, Sumei Zheng
The Higher Educational Key Laboratory for Flexible Manufacturing Equipment Integration of Fujian Province, Xiamen Institute of Technology, Xiamen 361000, China. · State Key Laboratory for Manufacturing Systems Engineering, Xi'an Jiaotong University, Xi'an 710049, China.
Key points
From the paper's conclusion- The results indicate that at glass powder contents of 2.94-10.22 wt%, the flexural strength of CBN blocks decreases by 32.5-89.4%, and binder microhardness reduces by 26.5-58.3%.
Abstract
Cu-Sn-Ti metallic-bonded CBN (Cubic Boron Nitride) abrasives are widely applied in the precision grinding of superhard materials. However, their high density and high toughness easily lead to poor grain protrusion and inadequate self-sharpening. In this work, ceramic glass powder was incorporated to modify the Cu-Sn-Ti binder, thereby fabricating composite-bonded CBN abrasive blocks with qualified mechanical properties and excellent self-sharpening performance. Flexural strength of abrasive blocks and microhardness of composite binders were measured; microstructure was characterized, phase composition was analyzed by XRD, and tribological tests were carried out between CBN blocks and silicon nitride abrasives. The results indicate that at glass powder contents of 2.94-10.22 wt%, the flexural strength of CBN blocks decreases by 32.5-89.4%, and binder microhardness reduces by 26.5-58.3%. At high brazing temperature, Ti and Cu from Cu-Sn-Ti alloy react with Si and Al in glass powder at the interface to form new phases including Ti2O3, Ti5Si3 and Ti(Cu,Al)2, which facilitates favorable interfacial bonding among the alloy matrix, glass phase and CBN grains. With increasing glass powder content, the strength decline gradually slows down. The overall wear resistance of abrasive blocks declines. SEM observations on worn CBN blocks and their composite binders reveal the formation of micropores within glass-containing binders, accompanied by a shift in the fracture mode of CBN abrasives upon glass powder addition. Comprehensive experimental analysis indicates that the No.3 sample with 8.33 wt% glass powder possesses the optimal overall performance.
Read the paper
Discussion
Science Skim's AI key points, plus readers' public thoughts
Readers' thoughts
No reader thoughts yet.
Related papers
- Improving the Performance Properties of Cutting Blades Through the Application of WC+5Co+TaC-NbC Nanocrystalline Composite MaterialMaterials · 2026
- Nanoparticle-induced phase transformation boosts mechanical and ablation performance of C/C–ZrC–SiC compositesJournal of Advanced Ceramics · 2026
- Microstructure and Grinding Performance of Resin‐Bonded Agglomerated Abrasives From KH550‐Modified Brown Fused AluminaInternational Journal of Applied Ceramic Technology · 2026
- Effect of Ti 3 SiC 2 and SiC on Mechanical and Tribological Properties of Copper Matrix Composites With Different ContentAdvanced Engineering Materials · 2026
- Effect of Boron Source on Microstructure and Mechanical Properties of SiBCN CeramicsJournal of the American Ceramic Society · 2026
- Mechanical Properties and Cutting Performance of Si 3 N 4 Ceramic Tools for CGI Turning at Different SpeedsInternational Journal of Applied Ceramic Technology · 2026