Effect of Compositional Tuning of Co Content on Microstructure Evolution and Property Optimization in CrFeNiAlSi High-Entropy Alloys.
Ying Wen, Shuang Meng, Guanyu Yang, Jian Chen
School of Mining, Liaoning Technical University, Fuxin 123000, China.
Key points
From the paper's conclusion- The results show that the HEA phase prediction results agree well with the experimental characterization, and all CrFeNiAlSiCo x HEAs exhibit a multiphase structure consisting of BCC and Cr3Si phases.
Abstract
To improve the comprehensive properties of CrFeNiAlSi HEA, CrFeNiAlSiCo x (x = 0.3, 0.6, 0.9, 1.2, molar ratio) high-entropy alloys (HEAs) with a multiphase structure were designed and fabricated by adding Co element. The phase compositions of the alloys were theoretically predicted based on the solid solution phase formation criteria. Combined with XRD, SEM, and EDS, the effects of Co content on the phase structure and microstructure evolution of the alloys were systematically investigated, and the hardness, wear resistance, corrosion resistance, and high-temperature oxidation resistance at 800 °C of the alloys were evaluated. The results show that the HEA phase prediction results agree well with the experimental characterization, and all CrFeNiAlSiCo x HEAs exhibit a multiphase structure consisting of BCC and Cr3Si phases. All alloys display a dendritic morphology, and the grain size is gradually refined with increasing Co content. The grain boundary regions are enriched with Si, the intragranular region consists of the AlNi phase, and the Co element is uniformly distributed across the grain boundaries and intragranular regions without obvious segregation. In terms of mechanical properties, the Co0.9 HEA exhibited the optimal hardness (1138.7 HV) and wear resistance (wear loss per unit area of 5.28 mg·cm-2). Regarding corrosion and oxidation performance, there is an optimal value for the effect of Co content: the Co1.2 HEA exhibited the lowest annual corrosion rate (0.014 mm/a) in a 3.5 wt % NaCl solution and the minimum weight gain (0.700 mg·cm-2) after oxidation in static air at 800 °C for 100 h, demonstrating the best corrosion resistance and high-temperature oxidation resistance.
Read the paper
Discussion
Science Skim's AI key points, plus readers' public thoughts
Readers' thoughts
No reader thoughts yet.
Related papers
- Silicon‐Induced Microstructural Refinement and Its Influence on Tribological and Corrosion Behavior of CoCrFeMnNi High‐Entropy AlloysAdvanced Engineering Materials · 2026
- High‐Entropy Alloy Design Toward Cobalt Substitution for High Hardness and Low Wear Rate Using X–Cr–Fe–Mn–Ni SystemAdvanced Engineering Materials · 2025
- A Review on Wear Behavior of High Entropy Alloys: Influence of Composition, Temperature, and Processing TechniqueJournal of Tribology · 2026
- High-throughput screening and Cu-content-driven optimization of properties in Cux(CoCrFeNi)100-x high-entropy alloysJournal of Materials Research and Technology · 2026
- The effect of heat treatment on the microstructure and wear resistance of CoCrFeNiNb0.45 high entropy alloy under different sintering statesJournal of Materials Research and Technology · 2026
- Synergistic B/Si Microalloying Induced Wear Resistance Improvement in FeCoNiCrCu High‐Entropy Alloy Coatings Prepared by Annular Oscillating Laser DepositionRare Metals · 2026